How can bubbles be avoided in the bead?
This fault points to various possible causes:
1. Bead too thick
Remedy:
Check bead, keep as small as possible
2. Inadequate venting
Remedy:
- Check vacuum (at least 100 mbar)
- Increase temperature before vent zone
- Reduce screw speed
3. Melt temperature too high (material decomposition)
Remedy:
Reduce processing temperatures and / or screw speed
4. Moisture
Remedy:
Predry material
back