ContactPrintSitemapSearchde | en | us | zh

How can streaking, haze and other irregularities be prevented inside the molding?

 

This faults to various possible causes:

 

1. Impurities, mixing with other thermoplastics

Remedy:

  • Completely wash out other thermoplastics
  • Clean (purge) the cylinder and screw with our cleaning agent PLEXIFIX® sp
  • Avoid contamination with other thermoplastics in the drier and / or conveyor system
  • Do not add regrind
  • Do not mix different grades of PLEXIGLAS® molding compound

 

2. Differences in wall thickness, sharp-edged transitions, poor plasticizing

Remedy:

  • Reduce injection speed
  • Increase mold temperature
  • Vary meld and nozzle temperature
  • Round off and thoroughly polish gate
  • Lower screw speed
  • Increase back pressure
  • Use cylinder with better plasticizing properties

 

 